It looks that you have selected a wrong screw for pet. pet need a screw with atleastl/d ratio 21 and shallow flight depth like in A type screws and extra power heater then normal machiene. barrier flight type screw is best for high plasticising ,melting requirement.

Fine
Poor
2005-9-1 3:03:13 By billal hussain
Barrel temperature profile wrong. Too cold in the rear and middle zones;
Cold spots in the nozzle or nozzle adaptor;
Cold spots in the hot runner;
Back pressure too low.

Fine
Poor
2005-6-29 21:31:54 By Kenplas
1
 
 

Post A Reply

Temporarily shut down, no new message, sorry.

Name:

Email:



Message:

(Max. 2KB)





Attachment:     (Max. 500kB, .RAR.ZIP.JPG.GIF only)
Verification:

This forum published since July 03, 2002. Renewed on June 22, 2005.

[Plastics Project] [Plastics Machinery] [Plastics Mold] [Discussion Forum] [Contact Kenplas]
Copyright © 2024 Kenplas Industry Limited, Hangzhou Kenplas Machinery Ltd.              Powered by Alentus.