1. Reduce PRE-BLOW Pressure;
2. Increase BLOW-DELAY (PRE-BLOW too early);
3. Increase stretch speed;
4. Adjust the clearance between tip of stretch rod and bottom mold to 1-1.5mm (when STRETCH-END is reached);
5. Wall thickness of preform body is not uniform (radial);
6. Stretch rod doesn''t focus on center of bottom mold (e.g. stretch rod is bent);
7. Reduce heating temperature of preform bottom.

Fine
3
Poor
2006-2-15 15:26:03 By Kenplas
1
 
 

Post A Reply

Temporarily shut down, no new message, sorry.

Name:

Email:



Message:

(Max. 2KB)





Attachment:     (Max. 500kB, .RAR.ZIP.JPG.GIF only)
Verification:

This forum published since July 03, 2002. Renewed on June 22, 2005.

[Plastics Project] [Plastics Machinery] [Plastics Mold] [Discussion Forum] [Contact Kenplas]
Copyright © 2024 Kenplas Industry Limited, Hangzhou Kenplas Machinery Ltd.              Powered by Alentus.